几种典型产品透过率     样品厚度:1mm

 


 

波长

合成

气炼熔融

电、连熔

JGS2-1

JGS2-2

JGS3-1电熔

JGS3-2连熔

190

86.42

73.84

71.02

75.73

68.35

200

86.88

75.16

74.81

77.16

73.94

210

88.51

79.90

78.89

81.59

79.92

220

89.09

85.69

85.24

85.79

85.53

230

89.58

87.57

87.61

86.61

87.58

240

89.90

87.58

87.75

85.51

88.15

250

90.12

88.64

88.77

87.04

88.93

260

90.46

90.11

89.97

89.42

89.92

280

90.89

90.82

90.79

90.45

90.74

300

91.14

91.15

91.02

90.84

91.11

350

91.49

91.45

91.33

91.12

91.49

400

91.72

91.75

91.63

91.44

91.70

500

92.08

91.99

91.89

91.68

92.04

750

92.26

92.32

92.13

91.91

92.26

1000

92.52

92.48

92.64

92.60

92.34

2000

93.25

93.48

93.51

93.52

93.26

2500

91.58

93.56

93.57

93.77

93.33

2600

87.06

92.45

92.38

95.59

94.91

2730

9.45

64.98

57.71

79.35

64.04

3000

89.70

91.04

92.10

92.94

92.36

3200

92.84

92.61

93.27

94.02

91.42